抄録
Ca-Ti-O films were prepared by MOCVD using Ca(dpm)2 and Ti(OiPr)2(dpm)2 precursors. The phases, composition and morphology of Ca-Ti-O films changed depending on the molar ratio of Ca to Ti precursors (RCa/Ti), total pressure (Ptot) and substrate temperature (Tsub). CaTiO3 films in a single phase were obtained at Tsub = 973 and 1073 K. CaTiO3 films prepared at 873 K had a dense structure and smooth surface. CaTiO3 films prepared at Tsub = 1073 K had complicated rough surface with a cauliflower-like texture. Hydroxyapatite (HAp) formed in 3 days on the CaTiO3 film prepared at Tsub = 1073 K.
本文言語 | English |
---|---|
ページ(範囲) | 301-304 |
ページ数 | 4 |
ジャーナル | Key Engineering Materials |
巻 | 352 |
DOI | |
出版ステータス | Published - 2007 1月 1 |
ASJC Scopus subject areas
- 材料科学(全般)
- 材料力学
- 機械工学